Abstract:To investigate the regulatory effect of 4H-SiC surface polarity on graphite film growth, graphite films were prepared via CVD at 1700 °C using MTS. The phase structure and micromorphology of the films were systematically analyzed, with the flexibility and conductivity of the exfoliated films verified. Results show that, governed by substrate polarity, the graphite film exhibits 2D layered growth on the Si-face with a thickness of ~1.94 μm; whereas it shows vertical columnar growth on the C-face reaching a thickness of ~8.11 μm with significantly increased defects. Specifically, the Si-face-grown graphite film displays an intrinsic conductivity of 1.5×10? S/cm, with no visible cracks at a bending diameter of 0.8 cm. After 100 continuous bending cycles, the film remains electrically continuous, with the resistance variation eventually stabilizing at ~33.7%. This study reveals the distinct microscopic growth behaviors on the different polar surfaces of the 4H-SiC substrate, confirming the inherent flexibility and conductivity of the Si-face-grown graphite film.